JOURNAL OF APPLIED ELECTROCHEMISTRY 22 (1992) 1129-1134
Pitting corrosion of polycrystalline annealed copper in alkaline sodium perchlorate solutions containing benzotriazole M. M. LAZ, R. M. SOUTO, S. G O N Z A L E Z , R. C. SALVAREZZA,* A. J. ARVIA*
Departamento de Qulmica Fisica, Universidad de La Laguna, Tenerife, Spain
Received 2 July 1991; revised 27 November 1991
The pitting corrosion of copper in alkaline solutions in the presence of benzotriazole (BTA) was investigated. The presence of BTA shifts the breakdown (Eb) and the repassivating (Ep) potentials positively with respect to the blanks. However, the shift of Ep becomes smaller than that of Eb, particularly at pH 9 and 11. Pitting corrosion involves the formation of crystallographic pits. The kinetics of the process fits a nucleation and growth mechanism involving instantaneous nucleation and 3D growth under charge transfer control. The spatial distribution of pits indicates that there is no marked influence of a pit on the nucleation and growth of other pits.
1. Introduction
Protection characteristics of anodic layers in relation to the corrosion and passivation of copper in aqueous solutions of different electrolyte composition were extensively investigated over a wide range ofpH [1, 2]. The structure of the passivating layers formed on copper in alkaline solutions in the absence of inhi- bitors was related to a composite duplex layer consist- ing of an inner Cu(I) oxide layer and an outer Cu(II) oxide layer [3-7], their stability and protective charac- teristics depending considerably on the applied poten- tial range and the composition of the solution. Accord- ingly, in the presence of agressive anions such as C1- and C104-ions a characteristic breakdown potential (Eb) of the passive layer associated with the initiation of copper pitting can be determined [2, 8, 9]. From the practical standpoint it is of interest to increase the value of Eb, for instance, by using inhibitors. In fact it is known that benzotriazole (BTA) is one of the most effective inhibitors for copper corrosion [10] in many aqueous environments [11-20]. BTA efficiency for copper protection increases with pH, and for alkaline solutions the protective characteristics last for a relatively long time [18].
The inhibition mechanism by BTA for copper cor- rosion involves the formation of a polymeric complex containing cuprous ions, [Cu(I)BTA], [14, 16, 17, 19, 21], as concluded from i.r. reflectance spectroscopy [14], X-ray photoelectron spectroscopy [19], scanning electron microscopy [20, 22], and surface enhanced raman spectroscopy [23-27] data. It has also been reported that the complex polymer is underlaid with a cuprous oxide layer to form a bilayer structure [22, 28, 29]. It is known that the copper electrodis- solution occurs at potentials more positive with increasing BTA concentration, and that the reaction
* Visiting professor: Consejo Nacional de Investigaciones Cientificas
mechanism is the same as that for copper in BTA-free solutions [30]. On the other hand, an alternative mechanism based on the adsorption of BTA on cop- per has also been advanced [15, 31].
The present work refers to the behaviour of copper in moderate alkaline sodium perchlorate solutions containing BTA at various pH, particularly in relation to the initiation of pitting corrosion of copper. A kinetic model based upon the nucleation and growth mechanism is presented for describing the breakdown of the protective layer formed on copper in the pres- ence of BTA.
2. Experimental
A three-electrode electrochemical cell was used. Working electrodes consisted of flat discs (0.3 cm dia.) obtained by cutting electrolytic copper rods. First, the electrode surface was mechanically polished by employ- ing a gradual sequence of fine-grained emery papers ranging from 30 to 5 #m grit. After cleaning and dry- ing, the copper specimens were annealed at 500 ~ C for 2 h under a few millimetres pressure of argon, follow- ing the procedure described in [32], to minimize residual mechanical stresses and to achieve a repro- ducible grain size distribution. Subsequently, the speci- mens were electropolished in 85% ortho-phosphoric acid at 0.3 Acm -2 for 5 to 10 rain. Finally, the electro- polished electrodes were rinsed thoroughly with water and dried in air. Each working electrode was mounted in a vertical rotating shaft and the contact between the disc surface and the solution was made through a hanging meniscus [33]. The potential of the working electrode was measured against a saturated NaC1- calomel electrode (SSCE). Potentials in the text are referred to the SSCE scale. A cylindrical platinum grid was used as counter electrode.
y Trcnicas of Argentina.
0021-891X �9 1992 Chapman & Hall 1129
1130 M.M. LAZ ET AL.
~: 0.3
1 - - X
O.C
0.3
pH 7
t
i I ''tl~ " j / i t
I / . . . . . . . ~' 2 . , /
~ " x I c l
I J I 1
L I I I I L'
p H 9
I I c
l i I I I ! I
I I t I
I
I t
I J J J
e I
I I I I L
Id
do
j l
p H 1 1
i
i i 1
I
j ' i i
i
i l,' J
I I C I J
I t I I I i u
I I I I I
-dr -o.3 o.o & -o.6 -d3 d3 -a6 -d3 o.o d3 E / V v s SSCE
Fig. 1. V o l t a m m o g r a m s of an annea led copper e lectrode at 0.01 V s - ~ in 1 M N a C I O 4 + x m M BTA at p H 7, 9 and 11; 25 ~ C. Solid lines, x = 1; do t ted lines, x = 0.
Measurements were made at 25.0 _+ 0.1~ Sol- utions were prepared from twice-distilled water and A.R. chemicals, and purged with argon prior to each run. The stock solution composition was 1 M NaC104 + x m M BTA (0.5 ~ x ~< 2), its pH being adjusted to either 7, 9 or 11 by adding diluted NaOH solution.
Each run was started by using a new copper speci- men and by recording a cyclicvoltammogram at 0.01Vs -1 between -0 .70 and 0.30V, to select the potential ranges most adequate for the application of the potentiostatic double step technique. The poten- tial routine applied to the working electrode consisted of a potential hold for 3 min at E~, a potential close to the HER threshold potential. Subsequently, the potential was stepped for 100s to Ek, a potential within the potential range of Cu(I) oxide formation. Finally, the potential was stepped to Es, the latter being set in the copper electrodissolution potential range to record the anodic current transients. The potential sequence fits the condition Ec < Ek < Es.
SEM micrographs of the copper electrode surfaces were obtained with an Hitachi S-450 scanning electron microscope (SEM) for beam energies in the 20 to 25 kV range.
3. Results
3.1. Voltammetry and breakdown potentials
In general, at the three pH values the voltammograms recorded at 0.01Vs -~ in 1M NaCIO4 (Fig. 1, dotted traces) and in I mM BTA + 1 M NaC104 (Fig. 1, full traces) exhibit two well defined potential ranges related to the passivity (region I) and to the corrosion of copper (region II). The positive going potential scan shows a very small current contribution in region I, and a rapid increase of the anodic current in region II when the positive going potential scan exceeds Eb. Region II extends to lower potentials in the negative going potential scan displaying the typical hysteresis loop of pitting corrosion with a crossing point at the
repassivation potential. In principle, the voltammetric behaviour for copper in these solutions is similar to that found for the breakdown of passive layers and initiation of pitting corrosion for a number of metals in aggressive environments [34-37].
The presence of BTA shifts the value of E b positively, this effect being more remarkable at pH 9. On the other hand, the comparison of the reverse potential scans show that the repassivation process tends to be independent of the presence of BTA at pH 9. Thus, at pH 7, in the presence Of BTA the value of Eb is 0.15 V and the hysteresis loop in the reverse scan extends to 0.08V. Likewise, when the potential scan enters region I, a small and broad cathodic current peak is recorded between 0.00 and - 0 . 1 0 V (peak L). At pH 9, the value of E b is close to 0.20 V and the reverse scan enters region I at 0.04V. In this case peak Ic becomes better defined, and another cathodic current peak appears at - 0.45 V (peak IIc). Finally, at pH 11 the same features are observed, Eb = 0.24V, the reverse scan enters region I at 0.05 V, and peaks Io and IIc are clearly observed, the potential of the former one being practically pH independent.
The cathodic peak I c can be assigned to the electro- reduction of Cu(II) from the bulk solution and a possible adsorbed monolayer of a Cu(I)BTA- com- pound. Otherwise, peak II~, lying at potentials more negative than -0 .35 V, can be related to the electro- reduction of a strongly adsorbed [BTA- Cu(I)] x layer formed during the preceding electroreduction process, yielding Cu + BTA at the copper surface. This interpretation agrees with previous work on copper electrodeposition from solutions containing copper ionic species in the presence of BTA [38-40], and the polarographic investigations on the Cu(II)-Cu(I)- Cu~ system in the presence of BTA [41, 42].
The influence of the inhibitor in extending region I, i.e. to decrease the rate of formation of soluble copper species, and to promote the onset of passivity, is clearly seen from a comparison of voltammograms run in the
P ITTING C O R R O S I O N OF P O L Y C R Y S T A L L I N E A N N E A L E D CO PPE R 1131
i i i
o tt~ ( I )
O.| \ @
O.1 o
log CH,
Fig. 2. Dependence orE b values with log c + both in the absence and in the presence of BTA.
presence and in the absence of BTA. In both cases the values of E b shift positively as the pH of the solution increases fitting a linear Eb against log cH+ relation- ship (Fig. 2) with the same slope which is close to 0.025 V/pH unit (Fig. 2).
3.2. Potentiostatic anodic current transients
The potentiostatic current transients were run by using copper specimens previously held at Ec = - 0.70V for tc = 3 min to attain the complete electro- reduction of the copper surface, subsequently kept at Ek = 0.00 V for tk = 100 S to form the anodic passive layer, and finally potential stepped to Es to record the corresponding anodic current transient. The value of E S was set in the 0.10 to 0.30 V potential range. Typical current transients are shown in Figs. 3-5 for pH 7, 9 and 11. In all cases the current increases steadily, the initial slope of the current transients increases with Es, and for the highest values of Es a current plateau is approached.
3.3. SEM micrographs
At the three pH's SEM micrographs of copper speci- mens anodised at Es > Eb show pit-free domains and others with a large number of small crystallographic pits distributed at random (Fig. 6), and stepped poly- hedrical surfaces, probably representing the proper bulk metal crystallographic lattice. Occasionally, pit
~1.5
0
X ""1.0
0.5
E s =0.28 V E
30 60 90 120 150 t ls
02
0.1
Fig. 3. Anodic current transients recorded at different E~ values in 1M NaC104 + lmM BTA at pH7. The symbols denote the experimental data and the solid lines correspond to the current transients calculated with Equations 3 and 5.
~ 20 0.1
~ ES 0 E k
"~ Ec
t ~" 4- 1.0 ~ 10
30 6 0 9 0 t / s
Fig. 4. Anodic current transients recorded at different E s values in 1M NaCIO 4 + lmM BTA at pH9. The symbols denote the experimental data and the solid lines correspond to the current transients calculated from Equations 3 and 5.
overlapping is also observed. The pit size is rather uniform with an average pit diameter of about 3.8 #m, suggesting that the initiation of pitting implies a prob- able instantaneous nucleation. The pit-free domains at the copper surface appear to be covered by a micro- crystalline layer exhibiting the same topography as that already described for thick Cu-BTA films formed on copper [22].
4 . D i s c u s s i o n
4.1. General features of BTA as Cu corrosion inhibitor
The outer passive layer produced on copper immersed in aqueous solutions containing BTA at neutral and moderate alkaline pH values, in the absence of C1 ions, has been described as a polymeric, coherent and continuous film which is represented by the Cu(I) BTA basic stoichiometry [13, 14, 17, 20]. This layer is formed by the irreversible chemisorption of BTA in solution on the copper surface. In agreement with results previously reported for copper corrosion inhibition by the presence of BTA in 1% NaC1- containing solutions [21], the present data confirm that the optimum efficiency of the inhibitor appears at pH 9. The loss of inhibiting efficiency at pH 11 may be due to the fact that in this case either the passivating layer is not completely coherent or that it changes the
<
0
0.5
o2o~ Ek
EC
t P
~ " Es,O.30 V .
10 20 30 40 I t s
100
50
Fig. 5. Anodic current transients recorded at different E~ values in IM NaC104 + lmM BTA at p H l l . The symbols denote the experimental data and the solid lines correspond to the current transients calculated from Equations 3 and 5.
1132 M . M . L A Z E T A L .
Fig. 6. SEM micrographs of an annealed copper specimen after anodising for 100 s in I M NaC104 + 1 mM BTA. (a-d) p H 7, E s = 0.23 V; (e) p H 9 , E s = 0.24V; (f) p H = 11, E S = 0.25V.
PITTING CORROSION OF POLYCRYSTALLINE ANNEALED COPPER 1133
structure to become, to some extent, permeable to OH- ions and oxygen.
Otherwise, the comparison of the hysteresis loops obtained at different pH's suggests that the reforming of the passivating layer becomes faster at low pH. As the pH increases it appears that the competition between OH--ions and BTA as film forming species moves in favour of the former. This is in agreement with previously reported data for BTA-benzylamine- water-methanol systems where the formation of thicker copper oxide underlayers takes place at the higher pH without improving the inhibiting efficiency of the passivating layer [21].
Despite the inhibiting properties of BTA for copper corrosion, the present results show that C104- containing solutions can produce rupture of the passi- vating layer formed on copper in the presence of BTA, at all pH's when the value of Eb is exceeded.
4.2. Phenomenological description o f anodic current transients
The analysis of potentiostatic current transients allows exploration of possible mechanisms for copper pitting in BTA-containing solutions. For this purpose the nucleation and growth formalism can be used as a first approach to the problem.
Several current contributions can be considered in the current transients obtained at E~, namely, the current due to the double layer charging, the current related to the passive layer growth, the current for the base metal dissolution through the passive layer, and the copper pitting current. The sum of these contri- butions, Jr, expressed as apparent current densities jdl, Jp, Jd and jc, respectively, is
Jt = Jdl q ' - L q - J d q - J ' e ( 1 )
The double layer charging component quickly drops to zero so that in the time domain of the present study its contribution can be neglected. Moreover, as the copper specimens are anodised for 100 s in the passive potential range, the value ofjp can also be neglected. Thus Equation 1 reduces to
Jt = Ja + • (2)
On the other hand, as the contribution of the base metal electrodissolution is relatively small, this pro- cess can be modelled in the simplest way as the dif- fusion of copper cations from the metal surface through the passive layer to the bulk of the solution. Assuming a linear diffusion through a homogeneous thin passive layer, [43]:
Jd = P1 t-If2 (3)
with
PI = zFDt/2 Acrc 1/2 (4)
where D is the diffusion coefficient of copper cations through the passive layer and Ac is the difference in the cation concentration at both sides of the passive layer. The termja can be specifically related to the growth of
Table 1. Parameters resulting f rom the anodic current transient fit- tings by using Equations 3 and 5
p H E s P1 P2 P3 / V /mA s '/2 cm -2 /mA cm -2 /s -2
7.0 0.20 3.718 x 10 3 0.284 4.72 x 10 s
7.0 0.23 - 0.081 5.19 x I0 -4
7.0 0.28 - 1.401 1.28 • 10 3
9.0 0.12 1.55 • 10 .3 0.214 6.94 x 10 -5
9.0 0.18 - 0.351 9,39 x 10 .5
9.0 0.24 - 12.53 3.11 x 10 .4
11.0 0.20 0.0 13.11 1,78 x 10 4
11.0 0.25 - 13.26 2.19 x 10 4
I1.0 0.30 - 32.63 1.03 • 10 -3
the outer portion of the anodic layer during corrosion. The rate of accumulation of the outer portion of the anodic layer should depend onja, the solubility product of the Cu-BTA species and copper oxide-hydroxides formed at the different pH's, and on the diffusion rate of the soluble species towards the bulk of the solution. In the present case, due to the presence of BTA, result- ing in very low currents for the electrodissolution process, the protective characteristics of the passive layer must be emphasized. Only when Es lies close to E b, does the magnitude of the electrodissolution current approach that ofjc, being negligible for higher poten- tials. Therefore, under the present circumstances, since the contribution of the Jd term is not substantial, the influence of the electric field on the transport of copper ions through the passive layer can not be determined.
The apparent pitting current density, i.e., the Jc term, can be ascribed to the instantaneous nucleation and three-dimensional growth of conical pits under charge transfer control, as given by the following equation [44]:
= P2[1.0 - exp ( - - P 3 t 2 ) ] (5) L where
P2 zFk~c (6)
P3 = nM~cNosP -2 (7)
and k3c and k~c are the growth rate constants parallel and perpendicular to the metal plane, respectively, M S is the molecular weight of the salt whose density is p, and Nos is the number of sites available for nucleation. This model appears to be useful when the applied potential is sufficently greater than Eb- It should also be noted that for P3 => 0, then exp ( - P 3 t 2) ~ 1 - P3t 2 and Equation 5 leads to a simple relationship between Jc and t 2:
~ P2P3 t 2 ( 8 )
By using Equations 3 and 5, the current transients shown in Figs. 3-5 can be reproduced with the set of parameters depicted in Table 1.
The comparison of the present results with those recently reported for BTA-free C104-containing sol- utions at different pH's [37] show that the early stages of copper pitting in C104 -containing solutions can be described by a common mechanism independently of
1134 M . M . LAZ ET AL.
0.4 t ~ ,
0 . 3 -
o
0 . 2
0 . i
0 . 0 0 1 2 2 4 5 6
/'t?
Fig. 7. Pm against m plot for E~ = 0.23 V, pH 7.
the presence of BTA as inhibitor. However, for the latter case, the nucleation and growth process leading to crystallographic pits is exclusively under activation control, although the value of P3 is considerably lower than that reported for BTA-free CIO4 -ion containing solutions. This fact permits Equation 5 to be used in the former case as a linearized I against t 2 expression. The decrease of P3 can be assigned to a decrease in No due to the presence of BTA. As concluded from volta- mmetry and SEM data at pH > 7, the precipitation of CuBTA takes place atregions outside the pit domains.
4.3. S p a t i a l d i s t r ibu t ion o f p i t s
The spat ia l d i s t r ibu t ion o f pi ts fo rmed on the copper surface gives in fo rma t ion a b o u t ei ther the r a n d o m or the n o n - r a n d o m loca t ion o f pits on the copper co r rod- ing surface [45].
Assuming tha t pits are r a n d o m l y d i s t r ibu ted on the copper surface and tha t the p robab i l i t y (Pro) o f the number o f pi ts (m) occurr ing in a rb i t r a ry surface ele- ments o f the same size (AS). The value o f Pm is then given by the Poisson equa t ion [45]:
P,, = N m exp ( - - N ) / m ! (9)
where N is the average number o f pits in the a rea AS. In this case the value o f P,~ can be ca lcula ted f rom the exper imenta l results by dividing the number o f surface e lements con ta in ing m pits by the to ta l number o f e lements r a n d o m l y loca ted wi thin the specimen sur- face. The circles in Fig. 7 denote the exper imenta l probabi l i t ies , P,,, ob t a ined for p H 7 and Es = 0.23 V, and the solid line i l lustrates the co r re spond ing theor- etical d i s t r ibu t ion resul t ing f rom E q u a t i o n 9 with N = 1.60. These figures represent the exper imenta l ly found average n u m b e r o f pi ts co r r e spond ing to a surface e lement AS = 3.8 • 10-6cm 2.
In general, the reasonable agreement between theory and exper iment suggests tha t the a s sumpt ion o f a r a n d o m d i s t r ibu t ion o f pits in the exper imenta l system is correct . This implies tha t there is no m a r k e d influ- ence o f a pi t on the nucleat ion and growth o f o ther pits.
Acknowledgement
Financ ia l suppo r t for this work by the G o b i e r n o de
Cana r i a s (Direcci6n Genera l de Univers idades e Invest igaci6n) under C o n t r a c t No. 46/01.06.88, is gra teful ly acknowledged .
References
[I] U. Bertocci and D. Turner, in 'Encyclopedia of Electro- chemistry of the Elements', (edited by A. J. Bard), Vol. 2, Marcel Dekker, New York (1974).
[2] J. van Muylder, in 'Comprehensive Treatise of Electrochem- istry', (edited by J. O'M. Bockris, B. E. Conway, E. Yeager and R. E. White), Vol. 4, Plenum Press, New York (1981).
[3] H.D. Speckmann, M. M. Lohrengel, J. W. Schultze and H. H. Strehblow, Ber. Bunsenges. Phys. Chem. 89 (1985) 392.
[4] M.R.G. Chialvo, S. L. Marchiano and A. J. Arvia, J. Appl. Electrochem. 14 (1984) 165.
[5] M.R.G. Chialvo, Z. O. Zerbino, S. L. Marchiano and A. J. Arvia, ibid. 16 (1986) 517.
[6] J. G6mez Becerra, R. C. Salvarezza and A. J. Arvia, Electro- chim. Acta 33 (1981) 613.
[7] M. Wanner, H. Wiese and K. G. Weil, Ber. Bunsenges. Phys. Chem. 92 (1988) 736.
[8] M.R.G. Chialvo, R. C. Salvarezza, D. V~squez Moll and A. J. Arvia, Electrochim. Acta 30 (1985) 1501.
[9] M. Prrez Sfinchez, M. Barrera, S. GonzMez, R. M. Souto, R. C. Salvarezza and A. J. Arvia, ibid. 35 (1990) 1337.
[10] L. Horner and E. Pliefke, Wekstoffe und Korr. 33 (1982) 98. [11] J .B. Cotton, Proc. 2nd Int. Cong. Metallic Corrosion,
NACE, New York (1963) p. 590. [12] I. Dugdale and J. B. Cotton, Corros. Sci. 3 (1963) 69. [13] J.B. Cotton and I. R. Scholes, Brit. Corros. J. 2 (1967) 1. [14] G.W. Poling, Corros. Sci. 10 (1970) 359. [ 15] F. Mansfeld, T. Smith and E. P. Parry, Corrosion 27 (1971 ) 289. [16] F. Mansfeld and T. Smith, ibid. 29 (1973) 105. [17] R.F. Roberts, J. Electron. Spectroscopy 4 (1974) 273. [18] R. Walker, Corrosion 29 (1973) 290; 31 (1975) 97. [19] D. Chadwick and T. Hashemi, Corros. Sci. 18 (1978) 39. [20] T. Notoya and G. W. Poling, Corrosion 35 (1979) 193. [21] M. Fleischmann, I. R. Hill, G. Mengoli and M. M. Musiani,
Electrochim. Acta 28 (1983) 1325. [22] T. Notoya and G. W. Poling, Corrosion 32 (1976) 216. [23] J.J. Kester, T. E. Furtak and A. J. Bevolo, J. Electrochem.
Soc. 129 (1982) 1716. [24] J. Rubim, I. G. R. Gutz, O. Sala and W. J. Orville-Thomas,
J. Molec. Struct. 100 (1983) 571. [25] M. Fleischmann, I. R. Hill, G. Mengoli, M. M. Musiani and
J. Akhavan, Electrochim. Acta 30 (1985) 879. [26] M.M. Musiani, G. Mengoli, M. Fleischmann and R. B.
Lowry, J. Electroanal. Chem. 217 (1987) 187. [27] R. Youda, H. Nishihara and K. Aramaki, Electrochim. Acta
35 (1990) 1011. [28] W. Paatsch, Ber. Bunsenges. Phys. Chem. 81 (1977) 645. [29] R. Alkire and A. Cangellari, J. Electrochem. Soc. 136 (1989)
913. [30] D. Thierry and C. Leygraf, ibid. 132 (1985) 1009. [31] S.L.F.A. Da Costa and S. M. L. Agostinho, J. Electroanal.
Chem. 246 (1990) 57. [32] M.M. Laz, R. M. Souto, S. Gonz~lez, R. C. Salvarezza and
A. J. Arvia, Electrochim. Acta, 37 (1992) 655. [33] D. Dickertmann, F. D. Koppitz and J. W. Schultze, Electro-
chim. Acta 21 (1976) 967. [34] D.V. Vfisquez Moll, R. C. Salvarezza, H. A. Videla and
A. J. Arvia, Corros. Sci. 24 (i984) 75l. [35] C.A. Acosta, R. C. Salvarezza, H. A. Videla and A. J. Arvia,
ibid, 25 (1985) 291. [36] R.C. Salvarezza, N. de Cristrfaro, C. Pallotta and A. J.
Arvia, Electrochim. Acta 32 (1987) 1049. [37] R.M. Souto, M. Prrez S~inchez, M. Barrera, S. Gonzfilez, R.
C. Salvarezza and A. J. Arvia, Electrochim. Acta, 37 (1992) 1437.
[38] J.K. Prall and L. L. Shreir, Corros. Sci. 1 (1961) 181. [39] B.S. Sheshadri, J. Electroanal. Chem. 61 (1975) 353. [40] J.C. Rubim, I. G. R. Gutz and O. Sala, ibid, 190 (1985) 55. [41] F. Pergola, M. R. Moncelli and R. Gtfidelli, ibid, 107 (1980) 295. [42] M.L. Foresti, F. Pergola and R. Guidelfi, ibid, 107 (1980) 307. [43] B. Scharifker and G. Hills, Electrochim. Acta 28 (1983) 879. [44] M.Y. Abyaneh and M. Fleischrnann, Electrochim. Acta 27