OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing...
-
Upload
nguyenhanh -
Category
Documents
-
view
221 -
download
0
Transcript of OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing...
![Page 1: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/1.jpg)
OLEH :
AKBAR RIANIRI BAKRI
4108100108
DOSEN PEMBIMBING :
Wing Hendroprasetyo Akbar Putra,S.T.,M.Eng
![Page 2: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/2.jpg)
LATAR BELAKANG
KONDISI
KAPAL
BEROPERASI
BRACKET
KAPAL
(FILLET JOINT)
PEMERIKSAAN
NDT
ULTRASONIC
TESTING
KONSTRUKSI
WELDINGCRACK/RETAK
REPARASI/
PERBAIKAN
KONDISI
COATING
DETEKSI
RETAK
![Page 3: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/3.jpg)
PERUMUSAN MASALAH
Bagaimana perbandingan panjang dan kedalaman retak yang
sebenarnya setelah dilakukan beberapa variasi ketebalan
nonconductive coating) dengan menggunakan teknik 6dB drop
dan 20dB drop?
Bagaimana pengaruh variasi ketebalan nonconductive
coating terhadap sensitivitas pendeteksian panjang dan
kedalaman retak yang terjadi jika dilakukan pemeriksaan
dengan menggunakan teknik 6dB drop dan 20dB drop?
![Page 4: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/4.jpg)
MAKSUD DAN TUJUAN
Membuat sebuah SOP (standard operating procedure)
yang dapat digunakan oleh teknisi UT di lapangan dalam
menentukan panjang serta kedalaman retak secara pasti
dan akurat.
Mengetahui kemampuan pendeteksian dan penentuan
ukuran retak (panjang dan kedalaman) yang diakibatkan
penggunaan variasi ketebalan nonconductive coating)
dengan menggunakan teknik 6dB drop dan 20dB drop.
![Page 5: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/5.jpg)
MANFAAT
Diperoleh suatu petunjuk praktis untuk penentuan
efektifitas pendeteksian panjang cacat yang sebenarnya
setelah dilapisi nonconductive coating menggunakan
metode ultrasonic test.
Dapat diketahui perbandingan panjang cacat yang
sebenarnya setelah dilapisi variasi ketebalan
nonconductive coating dengan pemeriksaan ultrasonic
test.
![Page 6: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/6.jpg)
METODOLOGI PENELITIANMulai
Identifikasi
masalah
Studi literatur
Pengadaan dan Penentuan
Material Uji(Aluminium Alloy 5083 dan jenis nonconductive
coating)
Pembuatan Spesimen UjiSpesimen pelat (AA5083 ) 300x200x12mm sejumlah
4 buah.
Pengelasan Fillet Joint double bevel dengan sudut
30
Pembuatan cacat pada specimen dengan panjang 10
mm, 30 mm, 50 mm, dan 70 mm.
Pembuatan cacat pada specimen dengan kedalaman 2
mm, 4 mm, 6 mm, dan 8 mm.
Proses Pengerjaan Material
Persiapan permukaan
Lima variasi aplikasi ketebalan cat yaitu
tanpa cat, 100, 200, 250 dan 300 mikron.
Pengujian UT
Pengolahan Hasil
uji
Analisis Data
Kesimpulan
Referensi
![Page 7: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/7.jpg)
MODEL SPESIMEN UJI
![Page 8: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/8.jpg)
MODEL SPESIMEN UJI
100 mikron 200 mikron
300 mikron250 mikron
Variasi ketebalan
nonconductive coating
1. 100 mikron
2. 200 mikron
3. 250 mikron
4. 300 mikron
12 mm
12 mm 12 mm
12 mm
![Page 9: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/9.jpg)
PEMBUATAN CRACK
Master EDM
dengan bentuk
elips
Proses pembuatan
crack menggunakan
mesin EDM
![Page 10: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/10.jpg)
PERSIAPAN COATING
Persiapan alat dan pembersihan permukaan spesimen sebelum pengecatan
![Page 11: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/11.jpg)
PENGUKURAN KETEBALAN
![Page 12: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/12.jpg)
PERSIAPAN SCANNING
![Page 13: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/13.jpg)
METODE SCANNING
SCANNING METHOD ACCORDING TO
AWS D1.1,ANNEX S,FIGURE 7
![Page 14: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/14.jpg)
![Page 15: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/15.jpg)
Retak
Hd =Max
Hd/2Hd/2
Pemeriksaan Ultrasonic Testing untuk mendeteksi panjang retak
dengan teknik 6 dB drop.
![Page 16: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/16.jpg)
70 mm
20 mm10 mm
30 mm
Hasil pemeriksaan Ultrasonic Testing
dengan ketebalan 100 mikron
68,65 mm 28,96 mm
19,29 mm
9,22 mm
![Page 17: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/17.jpg)
Hasil pemeriksaan Ultrasonic Testing
dengan ketebalan 200 mikron
70 mm
20 mm 10 mm
30 mm
67,87mm
17,79
mm
27,94mm
7,9 mm
![Page 18: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/18.jpg)
Hasil pemeriksaan Ultrasonic Testing
dengan ketebalan 250 mikron
70 mm
20 mm10 mm
30 mm
7,38 mm
27,71 mm
17,27mm
67,23 mm
![Page 19: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/19.jpg)
Hasil pemeriksaan Ultrasonic Testing
dengan ketebalan 300 mikron
70 mm
20 mm 10 mm
30 mm
66,86 mm
7,11
mm
27,48 mm
16,86 mm
![Page 20: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/20.jpg)
No Panjang Aktual Retak
Buatan (mm) Sebelum
diberi variasi
nonconductive coating
Panjang Indikasi Retak
Buatan (mm) Setelah
diberi variasi
nonconductive coating
Presentasi (%)
kemampuan
pembacaan
UT
1 70 68,65 98,071
2 30 28,96 96,533
3 20 19,29 96,450
4 10 9,22 92,200
Rata-rata 95,814
Hasil pemeriksaan panjang retak dengan ketebalan
coating 100 mikron
ANALISIS DATA DAN PEMBAHASAN
![Page 21: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/21.jpg)
Hasil pemeriksaan panjang retak dengan ketebalan
coating 200 mikron
No Panjang Aktual Retak
Buatan (mm) Sebelum
diberi variasi
nonconductive coating
Panjang Indikasi Retak
Buatan (mm) Setelah diberi
variasi nonconductive coating
Persentase (%)
kemampuan
pembacaan UT
1 70 67,87 96,957
2 30 27,94 93,133
3 20 17,79 88,950
4 10 7,9 79,000
Rata-rata 89,510
ANALISIS DATA DAN PEMBAHASAN
![Page 22: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/22.jpg)
No Panjang Aktual Retak
Buatan (mm) Sebelum
diberi variasi
nonconductive coating
Panjang Indikasi Retak
Buatan (mm) Setelah diberi
variasi nonconductive coating
Persentase (%)
kemampuan
pembacaan UT
1 70 67,23 96,043
2 30 27,71 92,367
3 20 17,27 86,350
4 10 7,38 73,800
Rata-rata 87,140
Hasil pemeriksaan panjang retak dengan ketebalan
coating 250 mikron
ANALISIS DATA DAN PEMBAHASAN
![Page 23: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/23.jpg)
No Panjang Aktual Retak
Buatan (mm) Sebelum
diberi variasi
nonconductive coating
Panjang Indikasi Retak
Buatan (mm) Setelah diberi
variasi nonconductive coating
Persentase (%)
kemampuan
pembacaan UT
1 70 66,86 95,514
2 30 27,48 91,600
3 20 16,86 84,300
4 10 7,11 71,100
Rata-rata 85,629
Hasil pemeriksaan panjang retak dengan ketebalan
coating 300 mikron
ANALISIS DATA DAN PEMBAHASAN
![Page 24: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/24.jpg)
Ketebalan
Coating
(Mikron)
Kemampuan
Pembacaan UT
(%)
100 95,814
200 89,510
250 87,140
300 85,629
Ketebalan
cat
Kemampuan
Pembacaan UT terhadap
panjang retak
(%)
ANALISIS DATA DAN PEMBAHASAN
![Page 25: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/25.jpg)
ANALISIS DATA DAN PEMBAHASANGRAFIK PERBANDINGAN KEMAMPUAN
PEMBACAAN PANJANG RETAK DENGAN
KETEBALAN COATING
95.814
89.510
87.14085.629
8384858687888990919293949596979899
100
0 50 100 150 200 250 300 350
Kem
am
pu
an
Pem
baaan
UT
(%)
Ketebalan Coating (mm)
Perbandingan Kemampuan Pembacaan panjang retak dengan ketebalan Coating
Perbandingan Kemampuan Pembacaan UT dan Ketebalan Coating
![Page 26: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/26.jpg)
ANALISIS DATA DAN PEMBAHASAN
Analisis Varians satu arah pengaruh ketebalan
nonconductive coating terhadap pembacaan
Panjang retak.
F Hitung > F Crit sehingga H0 ditolak. Dengan hasil
ini, berarti bahwa ketebalan nonconductive coating
berpengaruh terhadap pembacaan panjang retak
menggunakan metode ultrasonic testing (UT).
Panjang retak F Hitung F crit
70 2664.68 3.47805
30 7373.727 3.47805
20 6711.413 3.47805
10 4949.562 3.47805
![Page 27: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/27.jpg)
Dari hasil grafik perbandingan kemampuan pembacaan UT terhadap
variasi ketebalan coating dilakukan regresi sehingga di dapat persamaan :
y = -0.05x + 100.57
Persamaan ini dapat digunakan untuk menentukan
Persentase (%) kemampuan pembacaan UT pada
Ketebalan coating yang ingin dilakukan pemeriksaan
ANALISIS DATA DAN PEMBAHASAN
![Page 28: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/28.jpg)
RUMUS :
A=B*C(%)+B
A : Actual Crack (mm)
B : Indikasi Crack (mm)
C : selisih Kemampuan pembacaan UT (%) (Decreasing)
C = (100%-Kemampuan pembacaan UT %)
Kemampuan pembacaan UT(%) : y = -0.05x + 100.57
ANALISIS DATA DAN PEMBAHASAN
![Page 29: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/29.jpg)
![Page 30: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/30.jpg)
ANALISIS DATA DAN PEMBAHASAN
Pemeriksaan Ultrasonic Testing untuk mendeteksi kedalaman retak
80% FSH
8 % FSH
Retak
![Page 31: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/31.jpg)
Hasil pemeriksaan kedalaman retak dengan ketebalan
coating 100 mikron
ANALISIS DATA DAN PEMBAHASAN
No Kedalaman Aktual
Retak Buatan (mm)
Sebelum diberi variasi
non conductive coating
Kedalaman Indikasi Retak
Buatan (mm) Setelah diberi
variasi nonconductive coating
Persentase (%)
kemampuan
pembacaan UT
1 8 7.97 99.625
2 6 5.97 99.500
3 4 3.95 98.750
4 2 1.98 99.000
Rata-rata 99.219
![Page 32: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/32.jpg)
ANALISIS DATA DAN PEMBAHASAN
Hasil pemeriksaan kedalaman retak dengan ketebalan
coating 200 mikron
No Kedalaman Aktual
Retak Buatan (mm)
Sebelum diberi variasi
nonconductive coating
Kedalaman Indikasi Retak
Buatan (mm) Setelah diberi
variasi nonconductive coating
Persentase (%)
kemampuan
pembacaan UT
1 8 7.9 98.750
2 6 5.92 98.667
3 4 3.91 97.750
4 2 1.95 97.500
Rata-rata 98,167
![Page 33: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/33.jpg)
ANALISIS DATA DAN PEMBAHASAN
Hasil pemeriksaan kedalaman retak dengan ketebalan
coating 250 mikron
No Kedalaman Aktual
Retak Buatan (mm)
Sebelum diberi variasi
nonconductive coating
Kedalaman Indikasi Retak
Buatan (mm) Setelah diberi
variasi nonconductive coating
Persentase (%)
kemampuan
pembacaan UT
1 8 7.88 98.500
2 6 5.87 97.833
3 4 3.89 97.250
4 2 1.92 96.000
Rata-rata 97,396
![Page 34: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/34.jpg)
ANALISIS DATA DAN PEMBAHASAN
Hasil pemeriksaan kedalaman retak dengan ketebalan
coating 300 mikron
No Kedalaman Aktual
Retak Buatan (mm)
Sebelum diberi variasi
nonconductive coating
Kedalaman Indikasi Retak
Buatan (mm) Setelah diberi
variasi nonconductive coating
Persentase (%)
kemampuan
pembacaan UT
1 8 7.86 98.250
2 6 5.85 97.500
3 4 3.85 96.250
4 2 1.89 94.500
Rata-rata 96,625
![Page 35: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/35.jpg)
Ketebalan
cat
Kemampuan
Pembacaan UT terhadap
kedalaman retak
(%)
ANALISIS DATA DAN PEMBAHASAN
Ketebalan
Coating
(Mikron)
Kemampuan
Pembacaan UT
(%)
100 99,22
200 98,17
250 97,40
300 96,63
![Page 36: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/36.jpg)
ANALISIS DATA DAN PEMBAHASAN
GRAFIK PERBANDINGAN KEMAMPUAN
PEMBACAAN KEDALAMAN RETAK
DENGAN KETEBALAN COATING
99.22
98.17
97.40
96.63
95
0 100 200 300Ke
mam
pu
an
Pem
baaan
UT
(%)
Ketebalan Coating (mm)
Perbandingan Kemampuan Pembacaankedalaman Retak dengan Ketebalan Coating
Perbandingan Kemampuan Pembacaan UT dan Ketebalan Coating
![Page 37: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/37.jpg)
ANALISIS DATA DAN PEMBAHASANAnalisis Varians satu arah pengaruh ketebalan
nonconductive coating terhadap pembacaan
kedalaman retak.
F Hitung > F Crit sehingga H0 ditolak. Dengan hasil
ini, berarti bahwa ketebalan nonconductive coating
berpengaruh terhadap pembacaan kedalaman retak
menggunakan metode ultrasonic testing (UT).
Kedalaman
retak
F Hitung F crit
8 16.58051 3.47805
6 25.84483 3.47805
4 13.18182 3.47805
2 8.025 3.47805
![Page 38: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/38.jpg)
Dari hasil grafik perbandingan kemampuan pembacaan UT terhadap
variasi ketebalan coating dilakukan regresi sehingga di dapat persamaan :
y = -0.012x + 100.5
Persamaan ini dapat digunakan untuk menentukan
Persentase (%) kemampuan pembacaan UT pada
Ketebalan coating yang ingin dilakukan pemeriksaan
![Page 39: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/39.jpg)
RUMUS :
A=B*C(%)+B
A : Actual Crack (mm)
B : Indikasi Crack (mm)
C : selisih Kemampuan pembacaan UT (%) (Decreasing)
C = (100%-Kemampuan pembacaan UT %)
Kemampuan pembacaan UT (%) : y = -0.05x + 100.57
![Page 40: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/40.jpg)
KESIMPULAN
2. Berdasarkan hasil analisis varians satu arah, diperoleh
hasil bahwa variasi atau penambahan ketebalan cat
berpengaruh terhadap kemampuan pembacaan panjang
dan kedalam retak menggunakan Ultrasonic testing (UT).
1. Keakuratan pembacaan panjang dan kedalaman retak
menggunakan pengujian Ultrasonik akan menurun
seiring dengan penambahan ketebalan dari
nonconductive coating. Hal ini disebabkan adanya
pelemahan energi (atenuasi) dan pengaruh dari near
field.
![Page 41: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/41.jpg)
SARAN
Penelitian selanjutnya dapat menggunakan variasi frekuensi
dan ukuran kristal probe yang berbeda, sehingga dapat
diketahui pengaruhnya terhadap pendeteksian panjang dan
kedalam retak dengan pengujian Ultrasonik.
![Page 42: OLEH : AKBAR RIANIRI BAKRI DOSEN PEMBIMBING : Wing ...digilib.its.ac.id/public/ITS-paper-26828-4108100108-Presentation.pdfBagaimana perbandingan. panjang. dan. kedalaman retak yang](https://reader030.fdokumen.com/reader030/viewer/2022040417/5d4db71188c99357088b8980/html5/thumbnails/42.jpg)
TERIMA KASIH